Cream Breaking Rust
⭐⭐⭐⭐⭐
Recipe
Custer Feldspar | 26.6 |
Silica | 18.2 |
Wollastonite | 10.5 |
Kaolin | 8.5 |
Talc | 2.3 |
Strontium Carbonate | 3.3 |
Frit 3134 | 30.6 |
- | =100 |
Red Iron Oxide (RIO) | 6 |
Tin Oxide | 13 |
Bentonite | 2 |
Specific Gravity ≈ 1.40
Notes:
Cream that breaks to rust.
Great coverage on most dark clay bodies.
Most subtle with 1/2 the Red Iron Oxide (3%)
Does not tend to run.
Does not tend to cover speckles in speckled clay, most specks show through as rust colored spots.
Recipe originally from The Complete Guide to Mid-Range Glazes by John Britt.
Clay Body Key:
BM- Laguna B-Mix 5
B3- Laguna B-3
FR- Laguna Frost
LF-Armadillo Longhorn Red (low fire)